Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® T7300EG10 LS BK23346 - PA*-GF50 - BASF

Material Data Center offers the following functions for Ultramid® T7300EG10 LS BK23346:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid T datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Glass-fiber reinforced, heat aging resistant injection molding grade with excellent surface quality based on semi-crystalline polyamides with partially aromatic content. The product can be characterized as compound with very high strength and stiffness even after moisture uptake.

Markets & applications
Automotive: structural parts, metal replacement, brake parts, interior, powertrain
E&E: electrical appliances, cell phones
Consumer goods: home appliances, consumer electronics, furniture fittings
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 7 / * cm³/10min ISO 1133
Temperature 275 / * °C -
Load 5 / * kg -
Molding shrinkage, parallel 0.5 / * % ISO 294-4, 2577
Molding shrinkage, normal 0.7 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 17700 / 16600 MPa ISO 527
Stress at break 255 / 210 MPa ISO 527
Strain at break 2.8 / 3 % ISO 527
Charpy impact strength, +23°C 108 / 100 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 90 / 88 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 15 / 15 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 14 / 14 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 255 / * °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 240 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 255 / * °C ISO 75-1/-2
Other propertiesdry / condUnitTest Standard
Humidity absorption 1.2 / * % Sim. to ISO 62
Density 1600 / - kg/m³ ISO 1183
Material specific propertiesdry / condUnitTest Standard
ISO Data
Viscosity number 134 / * cm³/g ISO 307, 1157, 1628
Test specimen productionValueUnitTest Standard
ISO Data
Injection Molding, melt temperature 310 °C ISO 294
Injection Molding, mold temperature 100 °C ISO 294
Injection Molding, injection velocity 200 mm/s ISO 294
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 110 °C -
Pre-drying - Time 8 h -
Processing humidity ≤0.15 % -
Melt temperature 300 - 320 °C -
Mold temperature 80 - 120 °C -
Maximum residence time 5 min -
Diagrams
Viscosity-shear rate , Ultramid® T7300EG10 LS BK23346, PA*-GF50, BASF
Shearstress-shear rate , Ultramid® T7300EG10 LS BK23346, PA*-GF50, BASF
Stress-strain , Ultramid® T7300EG10 LS BK23346 (dry), PA*-GF50, BASF
Stress-strain , Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Secant modulus-strain , Ultramid® T7300EG10 LS BK23346 (dry), PA*-GF50, BASF
Secant modulus-strain , Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Stress-strain (isochronous) 23°C, Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Creep modulus-time 23°C, Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Creep curve 23°C, Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Stress-strain (isochronous) 80°C, Ultramid® T7300EG10 LS BK23346 (dry), PA*-GF50, BASF
Creep modulus-time 80°C, Ultramid® T7300EG10 LS BK23346 (dry), PA*-GF50, BASF
Creep curve 80°C, Ultramid® T7300EG10 LS BK23346 (dry), PA*-GF50, BASF
Tensile modulus-temperature , Ultramid® T7300EG10 LS BK23346 (dry), PA*-GF50, BASF
Tensile modulus-temperature , Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Characteristics
Processing
Injection Molding
Delivery form
Pellets, Black
Special Characteristics
Heat stabilized or stable to heat
Features
Laser Markable
Applications
Automotive, Electrical and Electronical
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, Pre-drying, Temperature: 110 °C
Pre/Post-processing, Pre-drying, Time: 8 h

PROCESSING
injection molding, Melt temperature, range: 280 - 310 °C
injection molding, Melt temperature, recommended: 300 °C
injection molding, Mold temperature, range: 80 - 120 °C
injection molding, Mold temperature, recommended: 100 °C
injection molding, Dwell time, thermoplastics: 5 min
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.